Resources
Instruct us

Gas Turbine Compressor VGV Failure Investigation

CEERISK was instructed to investigate recurrent coating loss and fatigue cracking in the compressor variable guide vanes (VGVs) of two F-class gas turbines, establishing the damage mechanism and specifying the metallurgical programme needed to confirm the root cause.

 Sector Power generation: combined-cycle power and water desalination
 Asset Two F-class heavy-duty industrial gas turbines (16-stage axial compressor with inlet guide vanes and three VGV rows)
 Event Turbine trips on guide vane control fault, followed by discovery of cracked, deformed and coating-depleted VGVs; the same damage was then found on a second unit
 Instructed by Loss adjusters acting on behalf of property insurers and reinsurers
 CEERISK Team Principal Engineer (PE, CEng) as lead investigator; Metallurgical & Materials Scientist (PhD, CEng, FIMMM)
 Service Site attendance and evidence documentation; component examination; operational data and trend analysis; maintenance-history reconstruction; metallurgical review; root cause analysis (RCA); forensic test-programme design; expert report

 

Related webinar: Investigating Gas Turbine Failures

The Challenge: Guide Vane Trips and Cracked VGVs

During a return to base load after planned downtime of a heat recovery steam generator, the first unit (Unit A) tripped on an inlet guide vane and VGV fault. Shortly after restart it tripped again, this time on a mismatch between the guide-vane trim controller and the demand signal on the first VGV row. The operator brought forward a modified compressor major inspection. Visual and magnetic-particle examination identified VGV vanes with cracks, aerofoil deformation and loose or missing coating, and seven vanes were rejected.

A fleet-wide inspection followed. It found similar coating loss on all three VGV rows of a second unit (Unit B). Once that unit was opened, several vanes were found to be cracked.

Insurers needed an independent answer to three questions: what damage had occurred, by what mechanism, and why. The answers would determine whether this was a sudden and accidental event or the end point of a progressive, known condition. Compressor-blade liberation in a heavy-duty gas turbine can cause extensive downstream damage, so the investigation also had to tell the operator whether the remaining fleet was at risk.

Download this Case Study

Keep this case study to hand. Download a single-page summary for your files.

Download PDF

CEERISK’s Approach: Hypothesis-Led Root Cause Analysis

CEERISK applied a structured, hypothesis-driven methodology consistent with the practice for investigating physical component failures in ASTM E2332 and the RCA principles in IEC 62740. The scientific method, as used in forensic engineering (NFPA 921), governed each stage: collect data, define the problem, form candidate hypotheses, test each one against the physical and documentary evidence, and form opinions only on what survives that testing. Evidence was collected, documented and preserved in line with ASTM E1188 and ASTM E860. This kept the evidential value of the parts intact for any later laboratory testing or dispute.

A single combined investigation was run for both units. The decision was made early, once the preliminary inspection had shown that both turbines had the same type of damage, most likely from a common cause. This reduced cost and duplication for the instructing insurers and allowed the second unit to be read against the first.

Six-stage methodology for a gas turbine compressor failure investigation, from evidence preservation to metallurgy and root cause analysis
Figure 1: CEERISK’s six-stage investigation methodology

Compressor Failure Investigation Steps

Scoping, Information Request and Evidence Preservation

Within days of instruction, CEERISK issued a targeted request for information (RFI). It asked for operating trends before, during and after both trips; alarm and event logs; the operator’s and manufacturer’s inspection reports; and records of earlier outages. The RFI was written around the candidate failure modes, not as a general document request, so that each item returned could confirm or exclude a hypothesis.

Site Attendance and Examination of Rejected Components

CEERISK’s Principal Engineer attended the plant with the insurers’ engineering loss adjuster. He held technical meetings with the operator’s engineers, the control-room team and the manufacturer’s site engineer, and examined the rejected vanes from both units directly.

  • Unit A had already been reassembled. Its six rejected Row 1 VGV vanes, palletised and quarantined on site, were examined one by one and photographed.
  • Unit B had its rotor removed and the vanes were still being cleaned for non-destructive testing (NDT). The rejected vanes from all three VGV rows were documented in their as-found state, before any further cleaning could change the surface evidence.

The same damage pattern was recorded on both units:

  1. Varying degrees of coating loss along the full length of the leading edge, on both the pressure and suction surfaces.
  2. Coating loss on the curved groove surfaces below the trunnion at the vane tip.
  3. Aerofoil deformation and surface roughening where the coating had been lost.
  4. Cracks and fractures directly below the tips and trunnions.
  5. Heavy black, oily soot deposits on aerofoil surfaces.

Row 1 compressor variable guide vane with leading-edge coating loss and crazing of the exposed surface
Figure 2(a) Unit A, Row 1 VGV: leading-edge coating loss with crazing of the exposed surface

Serrated coating-loss boundary on a compressor variable guide vane, typical of progressive spallation
Figure 2(b) Serrated coating-loss boundary, typical of progressive spallation

Crack running from the groove radius below a VGV trunnion into a coating-depleted zone
Figure 2(c) Crack running from the groove radius below the trunnion into a coating-depleted zone

Cracks initiating immediately below the trunnion of a compressor variable guide vane
Figure 2(d) Unit B: cracks initiating immediately below the trunnion

Figure 2(a,b,c,d): Representative as-found evidence documented by CEERISK on both units

Operational Data and Trend Analysis

CEERISK reviewed about 15 months of Unit A trend data leading up to the outage. The data covered power output, terminal voltage, shell temperature, combustor shell pressure, compressor inlet temperature, average exhaust temperature, barometric conditions, and relative and seismic vibration at the turbine inlet and exhaust bearings. No anomaly was found that would point to a sudden external event or an abrupt mechanical upset over that period. The high-resolution records from the two trip events showed the temperature fall and vibration response at the moment of each trip. These were consistent with the control system reacting to a guide-vane fault rather than causing one. This evidence weighed against a single sudden event as the initiating cause.

Reconstruction of the Maintenance and Inspection History

CEERISK obtained the manufacturer’s inspection reports for both units going back to 2018 and reviewed them critically. The aim was to establish when the condition first appeared, how it developed, and what was known and recommended at each stage. Performance and integrity degradation in industrial gas turbines is usually cumulative, so the history of a component is often as diagnostic as its final condition.

PeriodUnitKey findings relevant to the VGVs
2018Unit ABlack oily deposits on all blades and vanes; leading-edge coating erosion across rows; scaling and flaking on rotor discs; lube-oil leakage at casing joints. Repeated offline detergent washes recommended.
2018Unit BVGV borescope inspection: cracks and coating loss on all Row 1 VGVs; sliding contact and scoring on Row 2 and Row 3 trunnions. Rows 2 and 3 replaced with vanes from another unit.
2019Unit A“VGV mitigation” outage: Rows 1–3 cleaned and runout-checked; several aerofoils replaced; vanes partly sourced from another unit; trunnion-side machining.
2020Unit BCombustor inspection: leading-edge coating loss on inlet guide vanes; black residue on all VGV rows; no cracks seen by borescope.
2020Unit AShutdown inspection: borescope re-inspection recommended within 10 starts or 4,000 equivalent base-load hours.
2021Unit AModified major inspection after the trips: coating loss, leading-edge erosion with embedded material, fouled and rusted bushings, worn turnbuckle joints; seven vanes rejected.
2021Unit BFleet inspection found coating loss on VGV1–3; major inspection identified cracked vanes.

Table 1: Chronology of VGV-related findings reconstructed by CEERISK from inspection records

The chronology showed that the damage found in 2021 was consistent with, and similar to, conditions recorded at earlier inspections as far back as 2018. CEERISK also established that the manufacturer had revised the vane design and coating, and had recommended fleet replacement with the updated parts under an interim inspection regime. Neither affected unit had received the upgraded vanes when the damage was found; their replacement was scheduled for later that year.

Metallurgical Review of Crack Initiation

CEERISK’s Metallurgical & Materials Scientist examined the full photographic record of the vane surfaces and fracture regions from both units. He confirmed that the vanes from the two turbines had failed in the same way. Coating and plating loss was concentrated on the leading edges and on the grooved sections below the trunnion. Cracks had initiated at high-stress locations on the rounded grooves below the trunnions, mainly where coating loss was greatest. That pairing of crack origin and coating-depleted stress concentration is a well-established feature of fatigue cracking in compressor aerofoils, where surface degradation lowers fatigue strength at geometric stress raisers.

Failure-Mechanism Analysis and Hypothesis Testing

The physical evidence was assessed against the recognised degradation mechanisms for gas turbine flow-path components: solid-particle erosion, fouling, aqueous corrosion, hot corrosion and oxidation, and foreign-object damage. In an arid environment carrying airborne sand, dust, salts and phosphate particulates, erosion by particles above about 10 µm is a recognised and aggressive mechanism. It raises surface roughness, changes aerofoil geometry and removes protective coatings. Fouling by oil mist and soot, as recorded on both units, makes surface deposits more corrosive.

Every candidate explanation for the coating loss was kept open and tested against the evidence. None was ruled in or out on assumption. Table 2 shows the hypothesis matrix used.

Candidate cause of coating lossEvidence assessedDiscriminating test specified
(a) Deficient coating application in manufactureCoating loss recurring across units and outages; the manufacturer later revised the vane design and coatingCoating thickness against specification on metallographic cross-sections; examination of the coating–substrate interface for gaps, porosity and contamination
(b) Impact of loose abrasive debris at high rotational speedLeading-edge erosion and embedded material along the vane span; particulate-laden intake air; hard coating debris is itself abrasiveScanning electron microscopy (SEM) surface topography; energy-dispersive X-ray spectroscopy (EDX) of embedded particles to tell intake-derived debris from coating-derived debris
(c) High mechanical stress from vibrationCrack origins at stress concentrations below the trunnion; trunnion scoring and joint wear; no anomaly in the long-term vibration trendsFractography for fatigue features (beach marks, striations) and initiation sites; microhardness profiles
(d) Corrosion from fouling acting on either side of the coatingBlack oily soot, lube-oil leakage, surface rust on bushings and journals, salt-laden atmosphereEDX elemental mapping and chemical analysis of residues (e.g. S, Cl, Na); interface examination for under-coating attack

Table 2: Hypothesis matrix linking each candidate cause to evidence and to the test that discriminates it

 

Need to share this case study with your team? Download the one-page summary. Download PDF

Forensic Testing Programme

Visual and photographic evidence cannot, on its own, separate the four candidate causes, and CEERISK did not offer an opinion beyond what the evidence supported. It therefore specified a laboratory programme to confirm the root cause. Each test in the programme answers a specific hypothesis in Table 2 and follows a recognised method so that the results can be defended and repeated.

ExaminationMethod and purposeGoverning standard / reference
Surface topographyVisual and low-power stereomicroscopy of adherent coating and of the substrate where coating has been lost; digital imaging at graded magnificationsASTM E1188; ASM Handbook Vol. 12
SEM / EDXHigh-magnification imaging; EDX elemental analysis and colour dot-mapping to identify foreign or corrosive species on the surfacesASTM E1508
FractographyFracture faces opened by sectioning; examined visually, by stereomicroscopy and by SEM to establish initiation site, propagation mode and final fractureASTM E2332; ASM Handbook Vols. 11–12
Metallographic sectionsTransverse and longitudinal sections through coated and coating-free areas; mounted, ground to 1200 grit and polished to a 1 µm finishASTM E3
Coating thickness and interfaceOptical microscopy up to 1000× and SEM; thickness compared between locations and against specification; interface checked for gaps, porosity and impuritiesASTM B487 / ISO 1463
Microstructure and inclusionsChemical etching; base metal examined for cracks, voids and non-metallic inclusions and compared between locationsASTM E407; ASTM E45
HardnessHardness and microhardness profiles from the surface into the core, checked against the material specificationASTM E384 / ISO 6507-1
Residue analysisChemical analysis of deposits taken from different vane surfacesASTM E1508

Table 3: Forensic testing protocol specified by CEERISK

The programme was designed so that CEERISK’s experts could carry it out or witness it at the manufacturer’s laboratory or at an independent facility, under jointly agreed protocols. The site NDT on which component rejection relied (visual, magnetic-particle, liquid-penetrant and ultrasonic) was reviewed against the relevant practices, ASTM E709, ASTM E165 and ISO 9712 personnel certification, so that the rejection decisions themselves could be relied on.

Findings: Coating Loss and Fatigue Cracking

CEERISK’s opinions were stated to a reasonable degree of engineering certainty on the information available, with an express reservation to revise them if new evidence emerged, consistent with ASTM E620. The key findings were:

  • Common failure across both units. The rejected vanes from both turbines showed the same damage: coating loss on the leading edge and below the trunnion, cracks below the trunnion, surface roughening, erosion and corrosion of the exposed substrate, and heavy soot deposits.
  • Damage mechanism established. Cracks initiated at the stress-concentrating groove radius below the trunnion, preferentially where the coating had been lost. Without protective coating, the substrate is open to erosion, corrosion and loss of fatigue strength, and cyclic aerodynamic loading then drives crack initiation and growth (Figure 3).
  • A progressive, long-standing condition, not a sudden event. The same condition had been recorded at manufacturer inspections since 2018. Upgraded vanes and coatings had been recommended, but neither unit had received them at the time of the incidents, and both were running under an interim inspection regime meant to catch coating loss before it developed into cracking and vane liberation.
  • Root cause narrowed to four testable hypotheses. Four explanations for the coating loss were consistent with the evidence: application quality, abrasive debris impact, vibratory stress, and fouling-induced corrosion. A targeted metallurgical and chemical test programme was specified to determine which of them governs.

Damage pathway for compressor VGV fatigue cracking, from operating environment and coating degradation to crack initiation below the trunnion

Figure 3: Damage pathway and contributing factors established by CEERISK

Value Delivered

  • Clarity for insurers. A single, defensible account of both incidents, separating established fact from opinion. The maintenance chronology showed a progressive, pre-existing condition, which bears directly on how the claims are assessed.
  • Fleet risk visibility. The operator received an evidence-based explanation of why the interim inspection regime and the timely fitting of upgraded vanes were critical to preventing liberation and much larger downstream damage across the plant.
  • Efficiency. Treating both incidents as one investigation avoided duplicated site attendance and analysis while keeping each unit’s evidence distinct.
  • A clear route to the root cause. The test programme was proportionate and standards-based, linked each test to a hypothesis, and was ready for joint protocols with the manufacturer, so any further laboratory spend would be targeted rather than open-ended.

What Distinguishes the CEERISK Approach

Professional Standards Applied Throughout

  • Multi-disciplinary expertise: a chartered power-systems engineer working with a metallurgical and materials scientist, so that operational, mechanical and materials evidence were read together.
  • Independence and objectivity: opinions confined to the evidence and stated with an explicit degree of certainty. Where the evidence did not yet support a single root cause, CEERISK said so and specified the work needed. This is consistent with the overriding duty of an expert to assist the decision-maker, as in Civil Procedure Rules Part 35 and Practice Direction 35 (England & Wales).
  • Evidence integrity: as-found documentation before cleaning or disturbance, and preservation of rejected parts for later testing.
  • Hypothesis-led RCA: every plausible mechanism kept open and tested against physical, operational and documentary evidence.
  • Standards-based testing: each examination tied to a recognised ASTM or ISO method, so the results can be repeated and defended in a commercial or legal forum.

Related CEERISK Services

This engagement drew on CEERISK’s forensic engineering and metallurgical capabilities. CEERISK provides independent gas turbine compressor failure investigation and root cause analysis, site attendance and evidence preservation, metallurgical and materials analysis of failed components, review of operating data and maintenance history, and the design of standards-based forensic testing programmes. Findings are set out in expert reports prepared to be relied on in a commercial or legal forum.

Related services: Turbine, Compressor and Other Rotating Machinery, Metallurgy, Corrosion

Related webinar: Investigating Gas Turbine Failures

Investigating a Gas Turbine or Compressor Failure?

CEERISK provides independent forensic engineering investigation and root cause analysis across the power generation, energy and industrial sectors. If you need the cause of a gas turbine or compressor failure established, we welcome a discussion.

Contact Us